The compressive strengths of corrosion concrete with various temperatures.

Container numberSample numberTemperature (°C) (%)Compressive strength (MPa)Corrosion index K (%)
30 days90 days30 days90 days

L-165023.7326.3400
L-2620029.5930.1900
L-3640038.2438.9200
L-465520.0721.8915.4216.89
L-5620522.9121.8722.5727.56
L-6640528.8423.6624.5839.20
L-7651018.3119.8722.8424.56
L-86201020.3220.1231.3333.35
L-96401020.9521.0745.2145.86