Review Article
Recent Advances in the Deposition of Diamond Coatings on Co-Cemented Tungsten Carbides
Table 2
Wear resistance of the diamond coatings after laser and MP treatments.
| Sample | Worn surface, mm2 | Worn volume, mm3 | Max depth, m | Mean depth, m |
| 800 W | 21.6 | 0.0582 | 12.5 | 2.69 | 900 W | 14.7 | 0.0342 | 11.8 | 2.32 | 1000 W | 1.32 | 0.0185 | 5.77 | 1.4 | 1100 W | 1.29 | 0.0181 | 5.83 | 1.4 | 1200 W | 0.179 | 0.0019 | 4.64 | 1.08 | 1300 W | 0 | 0 | 0 | 0 | 1400 W | 0 | 0 | 0 | 0 | 1500 W | 0 | 0 | 0 | 0 | MP | 0 | 0 | 0 | 0 |
|
|