Research Article
Experimental Study on Formation Characteristics and Laws of Dislocation and Stacking Fault during Cutting of Titanium Alloy
Table 2
Mechanical and thermal physical properties of Ti6Al4V titanium alloy.
| Temperature/°C | 20 | 250 | 400 | 600 | 700 | 800 | 850 |
| Elastic modulus/GPa | 125 | 110 | 100 | 74 | 55 | 27 | 5 | Yield stress/MPa | 803.89 | 701.32 | 605.32 | 500.82 | 462.1 | 397.12 | 321.37 | Thermal expansion coefficient/10−6/·K | 8.78 | 9.83 | 10.68 | 11.42 | 12.01 | 12.21 | 12.37 | Thermal conductivity/W/m·K | 6.8 | 8.7 | 10.3 | 13.72 | 16.23 | 17.31 | 17.86 | Specific heat/J/Kg·K | 611 | 653 | 691 | 749.3 | 812.4 | 896.3 | 932.5 |
|
|