Loss rate of compressive strength of the carbonated AAS mortar.

ā€‰CarbonationCompressive strength of mortar (MPa)Area (mm2)Compressive strength of product (MPa) Loss rate of compressive strength (/)
ā€‰Period
(days)
Depth
(mm)
Before carbonation ()After carbonation ()Noncarbonation product ()Carbonation product ()Noncarbonation product ()Carbonation product ()

G774.036.733.7736176436.726.5172.2%
149.739.632.0156493639.627.4569.3%
2110.842.528.9169480642.522.4252.8%

G578.026.422.01344115626.418.2269.0%
1413.528.119.5197152928.117.1961.2%
2117.530.416.7227522530.415.3550.5%

G3718.012.57.5230419612.57.0756.6%
1425.013.17.22500013.17.2055.0%
2125.014.97.62500014.97.6051.0%