Research Article

Improvement in the Mechanical Properties of High Temperature Shape Memory Alloy (Ti50Ni25Pd25) by Copper Addition

Table 2

Yield stress, fracture stress, and fracture strain calculated from stress-strain curves of Figures 2 and 3 for Ti50Ni25Pd25 and Ti50Ni20Pd25Cu5 alloys.

AlloyPhaseTesting temperature (°C)0.2% Yield stress, (MPa)Fracture stress, (MPa)Fracture strain, (%)

Ti50Ni25Pd25Martensite69290951.610
Austenite2174401121.38.5

Ti50Ni20Pd25Cu5Martensite833231011.69.25
Austenite2285021162.27.3