Research Article

Electrospun Polyurethane/Loess Powder Hybrids and Their Absorption of Volatile Organic Compounds

Table 1

Physical properties of PU/LP spinning solutions.

Spinning solutionViscosity (cP)Fiber diameter (nm)BET area (m2/g)Tensile strength (MPa)
DistributionMean

PU + LP 0 wt%547290–9876365.99337.2 ± 2.31
PU + LP 10 wt%552290–9935261.34811.1 ± 0.05
PU + LP 30 wt%595184–6183432.60320.5 ± 0.03
PU + LP 50 wt%830172–7113682.2095