Research Article
Testing of Microalloyed Steel Quality under Creep Conditions for a New Intended Use
Table 2
Tensile testing under static conditions at elevated temperatures.
| | Material | H300LAD | H380LAD | 16Mo3 | C16E | | | | | | | | |
| 20 | 301 | 425 | 385 | 492 | 270 | 450 | 215 | 390 | 200 | 297 | 444 | 363 | 496 | 255 | 421 | 202 | 372 | 300 | 273 | 403 | 282 | 460 | 203 | 402 | 183 | 351 | 350 | 253 | 363 | 246 | 452 | 196 | 351 | 171 | 322 | 400 | 242 | 359 | 257 | 425 | 185 | 346 | 152 | 285 | 450 | 202 | 303 | 229 | 374 | 177 | 302 | 142 | 268 | 500 | 190 | 250 | 204 | 328 | 167 | 272 | 131 | 232 |
|
|
: temperature (°C); : yield strength (MPa); : ultimate strength (MPa).
|