Compressive strength of specified density shale aggregate concrete.
| Type | r (%) | Dry apparent density (kg/m3) | (MPa) | (MPa) | |
| Stone-LAC | 0 | 1330 | 35.8 | 24.7 | 0.69 | 25 | 1450 | 39.5 | 33.6 | 0.85 | 50 | 1550 | 41.5 | 35.4 | 0.85 | 75 | 1740 | 46.8 | 40.7 | 0.87 | 100 | 1940 | 55.6 | 47.3 | 0.85 |
| Sand-LAC | 0 | 1330 | 35.8 | 24.7 | 0.69 | 50 | 1510 | 42.1 | 35.9 | 0.85 | 100 | 1550 | 44.8 | 42.4 | 0.95 |
|
|