Results of the slow strain-rate tests performed at 45°C, total pressure of 800kPa, and 25% CO for different surface finishes.

SampleGrit finishElongationReduction in area

L52P120024.041.9
L70P120021.731.9
L68P80022.138.4
L59P60026.136.0
L57P40022.834.4
L67P40016.026.0
L63P22022.231.9
L66P18026.231.9