Research Article

Sealing of PEO Coated AZ91 Magnesium Alloy Using La-Based Solutions

Table 5

Quantitative results (at %) of EDS analysis of the samples before and after 7 days of immersion.

O%Na%Mg%Al%Si%P%La%Cl%S%

PEO61.042.5420.210.3412.423.45
12 g/l La 30°C 10 min60.622.3314.910.429.613.698.42
12 g/l La 50°C 30 min58.693.0612.430.969.424.2311.21
PEO Corr64.202.0019.200.39.472.501.11.23
12 g/l La 30°C 10 min Corr63.422.1218.260.38.962.422.540.961.02
12 g/l La 50°C 30 min Corr63.843.0012.360.47.672.799.560.150.23