Research Article
Three-Phase Characterization of Uniaxially Stretched Linear Low-Density Polyethylene
Table 2
Classical tensile properties (Elastic Modulus and Maximum Tensile force) and crystallinity by DSC of the oriented LLDPE monofilaments.
| Cold-draw ratio | E Modulus (MPa) | Max Tensile force (N) | DSC Crystallinity (%) |
|
A-3 | 7.2 | 270 ± 3 | 100 ± 9 | 51 ± 1 | A-4 | 6.1 | 203 ± 8 | 75 ± 5 | 50 ± 2 | A-5 | 5.7 | 165 ± 9 | 57 ± 4 | 47 ± 0 | A-6 | 5.0 | 144 ± 6 | 59 ± 6 | 47 ± 2 | A-7 | 4.5 | 125 ± 4 | 55 ± 5 | 47 ± 1 | A-8 | 4.2 | 112 ± 4 | 53 ± 2 | 46 ± 3 | A-9 | 3.7 | 103 ± 3 | 45 ± 3 | 46 ± 0 |
|
|