Research Article
Synthesis and Characterizations of Poly(trimethylene terephthalate)-b-poly(tetramethylene glycol) Copolymers
Table 4
Parameters of the TGA curves for the various samples.
| PTT/PTMEG (wt%/wt%) | (°C) | (°C) | (°C) | (%) | (Pa·s) | (MPa) | (%) | (KJ·m−2) | (Sh D) |
| C0-100/0 | 343.8 | 369.0 | 406.5 | 0.69 | 345.1 | 30.4 | 33.3 | 7.6 | 76 | C1-83/17 | 345.8 | 367.9 | 409.9 | 0.75 | 230.2 | 11.4 | 249.1 | 16.5 | 58 | C2-66/34 | 324.3 | 362.4 | 408.0 | 0.83 | 168.8 | 8.7 | 398.6 | 28.8 | 41 | C3-40/60 | 274.8 | 351.3 | 408.0 | 0.26 | 111.5 | 5.8 | 589.1 | 47.2 | 26 |
|
|
Tensile strength.
bElongation at breaking point.
cImpact strength.
dShore hardness.
|