Enzyme-Mediated Ring-Opening Polymerization of Pentadecalactone to Obtain Biodegradable Polymer for Fabrication of Scaffolds for Bone Tissue Engineering

Table 4

EMROP of pentadecalactone. Dependence of reaction time, yield, and intrinsic viscosity of resulting products on reaction temperature.

Sample numberT, °CTime, hYield, %[η], dL/g (GPC)* *

10356.03
11452.0870.30
12551.0870.5439.31.78
13651.5850.5629.11.58
14753.0890.59
15853.0900.75
16955.0860.79
171052.5911.0288.01.65
181152.0840.89

Here and further, the value corresponds to MW of a major eluted peak related to preliminary built calibration curve (polystyrene standards). Conditions: [M]/[E] = 10/1 wt./wt., [PDL] = 50 wt.%.