Research Article
Cure Cycle Effect on High-Temperature Polymer Composite Structures Molded by VARTM
Table 3
Process parameters effect on tensile strength for each case.
| Case number | Maximum cure temperature (°C) | Heating rate (°C/min) | Postcure time at 227°C (h) | Number of samples tested | Maximum tensile strength (MPa) |
| Case 1 | 194 | 1.39 | 2 | 5 | 856 | Case 2 | 194 | 0.56 | 2 | 5 | 825 | Case 3 | 183 | 1.39 | 2 | 5 | 884 | Case 4 | 205 | 1.39 | 2 | 5 | 817 |
|
|