Electrospun Polyamide 4.6 Nanofibrous Nonwovens: Parameter Study and Characterization
Table 3
The measured viscosity and conductivity for different PA 4.6 solutions.
| Concentration PA 4.6 (wt%) | Concentration acetic acid (v%) | Viscosity (mPa·s) | Conductivity (mS/cm) |
| 8 | 50 | 137 | 0.646 | 10 | 50 | 278 | 0.677 | 12 | 50 | 517 | 0.676 | 14 | 50 | 916 | 0.663 | 16 | 50 | 1434 | 0.621 | 18 | 50 | 2165 | 0.625 | 14 | 0 | 913 | 3.405 | 14 | 10 | 986 | 2.787 | 14 | 20 | 885 | 2.021 | 14 | 30 | 811 | 1.391 | 14 | 40 | 998 | 0.976 | 14 | 60 | 852 | 0.389 |
|
|