Research Article
Permeability of Electrospun Superhydrophobic Nanofiber Mats
Table 1
Electrospinning conditions of PFMOP.
| Polymer PFMOP to solvent concentration % wt/wt | Solvents | kV | Tip to collector Distance (cm) | Flow rate (mL/h) | Fiber diameter range (nm) | Log normal mean diameter (nm) | Log normal standard deviation |
| 1% |