Research Article
Freeze-Thaw Durability of Air-Entrained Concrete
Table 2
RDME of air-entrained concrete after different cycles of freeze-thaw (%).
| | Number of freeze-thaw cycles | | 0 | 50 | 100 | 150 | 200 | 250 | 300 | 350 | 400 |
| C20 | 100 | 99.45 | 99.4 | 98.75 | 96.7 | 83.85 | 64.95 | / | / | C25 | 100 | 97.60 | 94.35 | 91.55 | 90.75 | 77.35 | 62.8 | / | / | C30 | 100 | 99.55 | 98.75 | 98.2 | 94.6 | / | 93.9 | 87.3 | 77.05 | C40 | 100 | / | 98.4 | 98.55 | 99.05 | 98.9 | 97.35 | 96.75 | 95.4 | C50 | 100 | / | 95.85 | 97.6 | 97.5 | 95.8 | 90.35 | 85.95 | 77.6 |
|
|
“/” means: “the measurements were not made.”
|