7th-day and 28th-day and 90th-day CS and FS of marble and brick powder-blended and CEMI42.5N cement mortar samples [1].

Codes of mortarsCompressive strength (MPa)Flexure strength (MPa)
7th-day28th-day90th-day7th-day28th-day90th-day

CEMI42.5MP6M31.7640.7242.615.406.266.37
CEMI42.5MP20M26.9937.8232.314.845.435.30
CEMI42.5MP21M24.6132.5230.264.665.005.13
CEMI42.5MP35M21.8922.5522.044.104.123.88
CEMI42.5BP6M37.3542.7442.765.266.376.59
CEMI42.5BP20M37.5346.4151.736.097.048.60
CEMI42.5BP21M31.1843.9244.084.626.437.59
CEMI42.5BP35M27.7641.0544.364.707.218.32
CEMI42.5NM (Reference)31.7640.7242.615.406.26 6.37