Research Article

Research on Optimal Proportion and Performance of Cement-Clay Slurry

Table 7

Results of the orthogonal experiment.

Experiment numberDensityViscositySetting time (min)Water separation rate (%)Solidification rate (%)
InitialFinal

11.807.5012.830.299.5
21.806.5812.420.599.3
31.807.0012.251.098.3
41.797.5813.171.098.8
51.583211. 7520.924.295.0
61.563312.0821.252.593.3
71.502912.5021.753.193.3
81.533113.2523.084.293.3
91.442519.5830.087.086.3
101.432420.2531.085.191.3
111.452319.0829.2515.188.3
121.432220.7531.2513.087.5
131.322030.7547.9237.468.8
141.322031.2548.5830.571.8
151.321831.0848.1743.666.3
161.341831.5849.1730.572.0

Note. “—” means that the viscosity is very high and almost does not flow.