Single factor test.

Serial numberMass ratio of epoxy resin to curing agentMass ratio of phenolic amine to polyamideToughening agent dosage (%)Diluent content (%)Drawing strength (MPa)Shear strength (MPa)Bending strength (MPa)

12.01.5324.131.8459.66
23.01.5326.222.8975.69
34.01.5325.192.3462.3
45.01.5323.881.7748.6
53.01.0325.342.2372.5
63.01.5326.222.8978.36
73.02.0326.542.9580.69
83.02.5326.462.7781.1
93.01.5225.882.4476.2
103.01.5326.222.8980.36
113.01.5426.012.8477.6
123.01.5524.872.5669.1
133.01.5316.413.0479.65
143.01.5326.222.8975.6
153.01.5335.512.5568.45
163.01.5343.841.7654.14