Research Article

Influence of Codoping on the Optical Properties of ZnO Thin Films Synthesized on Glass Substrate by Chemical Bath Deposition Method

Table 1

The peak position, FWHM, average crystalline size, lattice constant, and average lattice strain for the (K, Fe) codoped ZnO thin films.

MaterialsPeak positionsFWHM of peaksAverage crystalline size (nm)Lattice constant (nm) Average crystalline strain (nm)
(100)(002)(001)(100)(002)(101)

K (1%)-Fe (1%)-ZnO film31.4934.1036.800.10880.10600.107677.390.30430.52700.0879
K (1%)-Fe (2%)-ZnO film31.9034.9036.900.11050.10950.108176.470.28620.49570.0882
K (1%)-Fe (3%)-ZnO film31.9034.9036.900.11020.10930.108876.080.30040.52030.0882