Process parameters combinations for high value of desirability.

FactorsPredicted responses
Exp. no. (µs) (µs)Ip (Ampere)SV (Volt)WF (m/min)WT (grams)MRR (mm3/min)Overcut (µm)Surface roughness (µm)Desirability

11.13816540414007.6329.202.430.603
21.0381604045007.4628.822.400.599
31.1381514345007.1428.112.440.589
41.0381664645007.5329.802.400.583
51.1331734045007.9831.212.490.579
61.130154401013947.7930.792.530.577
71.13814440513987.0028.152.470.577
81.12615140105008.4732.402.470.577
91.131157401013937.7930.812.390.576
101.02113040414009.1933.792.470.574
111.023145401014008.8733.282.370.573
121.12414640105008.8433.232.410.573
130.92115440414008.3832.372.450.573
141.12613740105008.1631.952.510.571
151.0281544095058.0831.892.440.568
161.138138431014006.7827.872.430.566
170.91814940414008.6933.272.480.564
181.12513840914008.4132.762.450.563
190.91716240414008.8433.742.450.558
200.9171524045008.9634.012.430.555
211.1381484147887.0729.652.430.553
221.12614248414007.6431.452.490.552
231.03815648411007.2030.552.430.543
241.0221484075008.5530.972.530.536
251.03817658105006.9430.452.470.527