Research Article
New Plaster Composite with Mineral Wool Fibres from CDW Recycling
Table 6
Tests of average results.
| ā | % waste addition | w/p | Bulk density (g/cm3) | Surface hardness Shore C | Flexural strength (MPa) | Compressive strength (MPa) |
| Reference | 0% | 0.6 | 1.226 | 89.867 | 7.272 | 17.352 | 0% | 0.8 | 1.014 | 75.400 | 4.247 | 8.708 |
| Recycled rock wool | 1% | 0.6 | 1.232 | 90.967 | 7.990 | 18.512 | 1.5% | 0.6 | 1.212 | 89.767 | 6.991 | 14.330 | 2% | 0.6 | 1.243 | 91.333 | 7.383 | 13.237 | 2.5% | 0.6 | 1.213 | 94.333 | 7.047 | 15.147 | 3% | 0.8 | 1.019 | 83.333 | 4.106 | 6.975 | 3.5% | 0.8 | 1.026 | 82.167 | 4.427 | 7.245 | 4% | 0.8 | 1.025 | 86.433 | 5.050 | 9.027 | 5% | 0.8 | 1.031 | 84.600 | 5.172 | 7.853 | 6% | 0.8 | 1.017 | 83.933 | 5.366 | 8.168 | 8% | 0.8 | 1.018 | 81.067 | 5.134 | 8.562 | 10% | 0.8 | 1.063 | 82.167 | 5.376 | 7.308 |
| Recycled glass wool | 1% | 0.6 | 1.238 | 92.333 | 7.263 | 16.613 | 1.5% | 0.6 | 1.206 | 90.100 | 6.686 | 12.295 | 2% | 0.6 | 1.199 | 90.433 | 6.373 | 12.017 | 2.5% | 0.6 | 1.200 | 90.900 | 6.722 | 11.200 | 3% | 0.8 | 0.999 | 78.933 | 4.283 | 6.110 | 3.5% | 0.8 | 1.004 | 81.333 | 4.113 | 6.559 | 4% | 0.8 | 1.009 | 83.867 | 4.673 | 8.153 | 5% | 0.8 | 1.011 | 81.567 | 4.599 | 7.315 | 6% | 0.8 | 1.020 | 81.567 | 4.869 | 7.240 | 8% | 0.8 | 1.045 | 83.133 | 5.046 | 7.542 | 10% | 0.8 | 1.056 | 80.800 | 5.707 | 7.522 |
|
|