Field investigation data (Building 7, construction completion year: 1983).

Measurement pointMember typeConcrete compressive strength (MPa)Concrete carbonation depth (mm)Cover depth (mm)Crack width (mm)

B7P1Slab25.27.6935
B7P2Beam18.610.3570
B7P3Slab25.511.7840
B7P4Beam26.47.3545
B7P5Beam31.411.36550.1
B7P6Slab32.17.8535
B7P7Column25.912.9030
B7P8Column26.38.7725
B7P9Beam25.111.9855
B7P10Slab25.213.3735
B7P11Beam26.07.8235
B7P12Slab22.09.8730
B7P13Slab20.012.31250.1
B7P14Beam27.511.0340
B7P15Slab19.98.0235
B7P16Beam24.513.3460
B7P17Wall19.717.8945
B7P18Wall20.520.35400.1
B7P19Wall24.418.4130
B7P20Wall21.623.06400.1