Table 2
Mix proportions of 400 kg/m3 GHBFC.
| Mixes designation | Design density (kg/m3) | Cement (g) | Fly ash (g) | GHBs (%) | Water-binder ratio | Foam (mL) |
| 400-fa | 400 | 1798 | 1199 | 0 | 0.60 | 5122 | 400-g1 | 400 | 1774 | 1199 | 0.8 | 0.60 | 5122 | 400-g2 | 400 | 1750 | 1199 | 1.6 | 0.60 | 5122 | 400-g3 | 400 | 1726 | 1199 | 2.4 | 0.60 | 5122 | 400-g4 | 400 | 1702 | 1199 | 3.2 | 0.60 | 5122 | 400-g5 | 400 | 1678 | 1199 | 4.0 | 0.60 | 5122 |
|
|
Note: the mixing amount of GHBs means the percentage of the gross binder material by weight.
|