Mechanical properties at room and high temperatures for each aging condition of all four alloys.
| Alloy number | Testing temp. (°C) | Yield strength (MPa) | Ultimate tensile strength (UTS) (MPa) | Underaged | Peak-aged | Underaged | Peak-aged |
| 1 | 20°C | 305 | 420 | 412 | 480 | 190°C | 315 | 350 | 354 | 372 | 250°C | 250 | 247 | 260 | 247 |
| 2 | 20°C | 260 | 275 | 366 | 385 | 190°C | 250 | 210 | 310 | 237 | 250°C | 200 | 190 | 214 | 195 |
| 3 | 20°C | 265 | 310 | 352 | 359 | 190°C | 190 | 250 | 220 | 271 | 250°C | 190 | 185 | 201 | 195 |
| 4 | 20°C | 300 | 400 | 405 | 447 | 190°C | 295 | 320 | 320 | 341 | 250°C | 200 | 210 | 220 | 245 |
|
|