Research Article

High- and Low-Temperature Properties and Thermal Stability of Silica Fume/SBS Composite-Modified Asphalt Mortar

Table 2

Results of DSR.

Test parametersTemperature (°C)Silica fume content (%)
1471013

(kPa)5819.820.09120.12520.15620.847
649.7169.84710.12310.23410.319
704.9665.0865.2225.2295.286
762.6932.7242.7712.7712.805
821.5311.5381.5441.5561.58

Δ (°)5876.1476.1275.5275.0774.33
6479.378.8177.677.1776.66
7081.4481.3379.8578.8978.39
7684.4683.8883.281.1979.66
8284.9484.7183.9782.5680.45

(/sin δ) (kPa)5820.39420.69520.78520.86021.652
649.88810.03810.47410.49610.605
705.0225.1455.3055.3295.396
762.7062.7402.7912.8042.872
821.5371.5451.5531.5691.602