Research Article

Microstructure and Density of Sintered ZnO Ceramics Prepared by Magnetic Pulsed Compaction

Table 2

Comparison of the grain sizes of the central and outer regions in the sintered specimens prepared using the three compacting methods (uniaxial pressing, CIP, and MPC).

Sintering temperature (°C)Compacting methodGrain size (m)
1 h2 h4 h
CenterSideCenterSideCenterSide

900Uni3.285 (no grain growth)
CIP
MPC

1100Uni6.6617.666.3418.477.3117.39
CIP7.9716.429.5917.9711.6419.41
MPC14.4416.7615.1319.0314.0623.50

1300Uni10.9818.2110.8520.2711.4625.89
CIP9.0218.8512.6523.0011.9424.71
MPC26.9429.2924.7137.3724.2934.29