Main properties of the geotextile (undamaged sample).

PropertyTest standardGeotextile

Mass per unit area (g·m−2)EN ISO 9864 [31]502 (±25)
Thickness at 2 kPa (mm)EN ISO 9863-1 [32]3.81 (±0.08)
Tensile strength MDa (kN·m−1)EN 29073-3 [33]26.64 (±1.41)
Elongation at the maximum load MDa (%)EN 29073-3 [33]71.6 (±3.2)
Tensile strength CMDb (kN·m−1)EN 29073-3 [33]13.43 (±1.03)
Elongation at the maximum load CMDb (%)EN 29073-3 [33]122.9 (±6.2)
CBR puncture resistance (kN)EN ISO 12236 [34]2.69 (±0.15)
Permeability (VIH50)c (mm·s−1)EN ISO 11058 [35]39.7 (±5.0)
Pore size (O90)d (m)EN ISO 12956 [36]66.0 (±4.9)

The 95% confidence intervals are given in parentheses; aMD, machine direction of production; bCMD, cross-machine direction of production; cVIH50, velocity index for a head loss of 50 mm; dO90, characteristic opening size.