Enrichment concentration values of Sample-C1 coal with Knelson method (−0.5 + 0.106 mm).

Rotational speedTest productWeight (%)Ash (%)Yield (%)Sulfur (%)

14 G (398 rpm)Concentrate56.0614.7626.002.97
Waste43.9447.1774.00
Feed sample10019.941003.24

24 G (530 rpm)Concentrate56.1316.8028.892.85
Waste43.8752.9071.11
Feed sample10019.941003.24

40 G (685 rpm)Concentrate60.6017.7938.373.13
Waste39.4043.9561.63
Feed sample10019.941003.24

60 G (839 rpm)Concentrate68.1015.9443.053.15
Waste31.9045.0256.95
Feed sample10019.941003.24

Feeds in the experiments are 100 g each.