Abstract

In this work, a new adsorbent with effective Pd(II) adsorption ability was synthesized using an oyster shell and fumed silica as the matrix materials and polyethyleneimine as the functional ligand. The adsorption performance of the developed adsorbent was evaluated for the recovery of palladium chloride ions (Pd(II)) from strong acid solutions. To understand the characteristics of the materials used in the study, samples were characterized by Fourier transform infrared spectroscopy (FT-IR), transmission electron microscopy (TEM), X-ray diffraction (XRD), and zeta potential analysis. Zeta potential analysis revealed that the isoelectric point of polyethylenimine-crosslinked calcium silicate hydrate (PEI-CSH) was 9.85. Isotherm experiments revealed that the maximum Pd(II) uptake estimated by the Langmuir model was 156.03 mg/g, which was 22.4 and 35.6 times higher than that of the oyster shell powder (OSP) and calcium silicate hydrate (CSH), respectively. The Pd(II) adsorption equilibrium was established in 180 minutes, according to kinetic experiments. These results suggested the possibility of Pd(II) recovery from oyster shell-based adsorbent. Through five adsorption and desorption cycles, the reusability of PEI-CSH was confirmed. PEI-CSH can therefore be considered a potential adsorbent for Pd(II) recovery.

1. Introduction

Palladium (Pd) has been widely used in automotive catalytic converters, jewellery, bimetallic catalysts, multilayer ceramic capacitors, fuel cell catalysis, and medical industries due to its unique properties [16]. With the rapid development of modern society, the demand for Pd is continuously increasing. But because of steady and constrained production, palladium is in greater demand than it is available [7, 8]. The ore only contains 2–6 g/t of Pd, but commonly phased out products like printed circuit boards and car catalytic converters have 100–10,000 g/t of Pd on average [9]. Therefore, the recovery of Pd from final items is therefore extremely important.

Leaching is commonly used to extract palladium from solid wastes, where large amounts of palladium-containing wastewater are generated. Recovery of Pd from wastewater is not only economically beneficial but also important in terms of public health, as excess Pd in water can have negative effects on human health. Consuming too much Pd can cause asthma, cancer, renal failure, and other illnesses [1012]. Some methods such as ion exchange [13], hydrometallurgy [14], and solvent extraction [15] have been used to recover and reduce the Pd concentration in wastewater; nonetheless, there are several drawbacks to these techniques, including high running costs and poor efficiency. Pd is thus transmitted from improperly treated industrial effluent that contains Pd to water bodies like rivers and lakes, having a negative impact on human and animal health. Therefore, it is vital to investigate low-cost and efficient Pd recovery techniques. Adsorption was therefore presented as a possible alternative for the recovery of palladium from wastewater since it overcomes the aforementioned drawbacks.

Natural materials often have complex hierarchical structures and thus can be used as adsorbent materials [16, 17]. A number of researchers have paid attention to the development of functional materials for environmental applications using agriculture [18], biological [19], and fermented [20] wastes. Oyster shell (OS) is an abundant biowaste that has attracted much attention [21]. It has been applied to remove heavy metals such as Ni(II) [22], Hg(II) [23], and Cd(II) [24] from wastewater. However, OS has low adsorption capacity and weak acid resistance, so there are limitations in treating acidic wastewater directly with OS. Aqua regia is commonly used to leach Pd from obsolete products, and the leachate is strongly acidic with large amounts of chloride ions. In order to use OS as an adsorbent for Pd recovery from acid solutions, the problem of low acid resistance must first be solved. Since OS (whose main component is CaCO3) and fumed silica can be converted to acid-insoluble calcium silicate hydrate (CSH) by calcination, the conversion of OS to CSH can be an effective way to compensate for the disadvantages of OS when it is used as an adsorbent [25]. In previous studies, the preparation of CSH involves the utilization of expensive and toxic chemical reagents [2628]. Here, OS, an abundant biowaste, was used to replace commercial calcium chloride and no toxic solvent was used in the preparation of CSH. Pd(II) exists mainly in the form of PdCl42- among several Pd-chloride complexes in strong acid solutions containing lots of chloride ions [29]. On the other hand, CHS synthesized from OS does not have a functional group capable of binding to PdCl42-. Therefore, it is necessary to apply appropriate surface modification methods to greatly improve the adsorption capacity of CSH towards Pd(II). An amine-rich polymer known as polyethylenimine has been extensively employed to alter adsorbents for the recovery of precious metals including P(II), Pt(IV), and Au(III) [9, 30, 31].

In this study, a polyethylenimine-crosslinked CSH (PEI-CSH) adsorbent for Pd(II) recovery was successfully prepared by crosslinking polyethylenimine (PEI) on the surface of CSH synthesized from OS. Characteristic properties of PEI-CSH were identified through FT-IR, XRD, zeta potential analysis, and TEM. The basic interaction between PEI-CSH and Pd(II) was confirmed by batch experiments. Adsorption isotherm experiments and kinetic experiments were also performed to investigate the adsorption ability of Pd(II) on PEI-CSH.

2. Materials and Methods

2.1. Materials

Palladium(II) chloride (purity: 99.0%) was purchased from Kojima Chemicals Co., Ltd. (Saitama, Japan). OS waste was collected from a local market in Tongyeong, South Korea. Branched PEI (: 70,000, content: 50%) was supplied by Habjung Moolsan Co., Ltd. (Seoul, Korea). 3-Aminopropyltriethoxysilane (APTES, 99%) was provided by Daejung Chemical & Metals Co., Ltd. (Siheung, Korea). Fumed silica was purchased from Sigma-Aldrich Korea Ltd. (Yongin, Korea). Glutaraldehyde (GA, 25% solution, extra pure) was supplied by Junsei Chemical Co., Ltd. (Tokyo, Japan). Other reagents such as ethanol, NaOH, and HCl used in this study were of analytical grade.

2.2. Preparation of PEI-CSH

To eliminate contaminants and silt, OS trash was first thoroughly cleaned with distilled water, followed by a day of drying in an air-drying oven. The washed OS was soaked in 5% sodium hypochlorite (NaClO) solution for 24 h to get rid of organic matters attached on the surface, then washed with distilled water, followed by a thorough drying. The dried OS was crushed by a ball mill (DW BM915, Dongwon Scientific System Co., Korea) with alumina balls at 500 rpm to produce oyster shell powder (OSP). The OSP (μm) was collected through sieving. In order to manufacture CSH, a 1 : 1.2 weight ratio of OSP and fumed silica was combined. This mixture was then calcined at 800°C for 6 h. [25].

PEI-CSH was prepared based on previously reported methods with slight modification [32, 33]. Briefly, CSH (3 g) and APTES (3 mL) were added to 300 mL of 30% ethanol 300 mL and stirred at 25°C for 24 h. Then, the APTES-treated CSH was collected by filtration, washed with ethanol several times, and dried overnight at 100°C. Finally, PEI-CSH was produced by mixing 1% PEI solution with APTES-CSH at 40°C for 24 h, during which 1 mL of 25% GA was added dropwise. The produced PEI-CSH was repeatedly washed in deionized water, dried for 24 hours in an oven at 40°C, and then kept in a desiccator for further use.

2.3. Analytical Methods

The IR spectra of OSP, CSH, and PEI-CSH were investigated using a FT-IR spectrometer in the range of 4000–400 cm-1 (Nicolet IS50, Thermo Fisher, USA). The compositions of OSP, CSH, and PEI-CSH were analyzed using XRD (D8 Advance A25, Bruker, USA) with Cu Kα radiation ( Å) and 2 range from 10° to 70°. A zeta potential analyzer was used to examine the zeta potential of CSH and PEI-CSH at various pH levels (ELSZ-2000, Otsuka, Japan). The surface morphologies of OSP, CSH, and PEI-CSH were observed by 300 kV TEM (Tecnai TF30, FEI, USA) at ×195,000 magnification.

2.4. Batch Adsorption and Desorption Experiments

The Pd(II) stock solution (1000 mg/L) was made by dissolving a particular amount of Pd(II) in 0.01 M HCl, and the Pd(II) concentrations used in this study were made by diluting the Pd(II) stock solution. Adsorption isotherm tests were conducted in the range of starting Pd(II) concentrations from 30 to 700 mg/L in order to determine the maximum adsorption capacity of the adsorbent for Pd(II). A shaking incubator was used to stir a 50 mL conical tube containing 0.06 g of adsorbent and 30 mL of Pd(II) solution for 24 hours at room temperature (25°C) and 160 rpm. Samples from the supernatant were taken after equilibrium to determine the final Pd content (II). At predetermined intervals during the kinetic studies, samples from the supernatant were taken for concentration measurement at an initial Pd(II) concentration of 200 mg/L. All the samples were taken in triplicate. The obtained samples were diluted accordingly with tertiary distilled water after being centrifuged for 10 min at 10,000 rpm. ICP-OES (Avio200, PerkinElmer, USA) was used to detect the residual Pd(II) concentration, and Equation (1) was used to determine the Pd(II) adsorption quantity (mg/g). where the initial and final Pd(II) concentrations, the working volume, and the weight of the adsorbent are expressed by and (mg/L), (L), and (g), respectively.

Prior to the desorption experiment, Pd(II)-loaded PEI-CSH was made by mixing 0.06 g of PEI-CSH with 30 mL of 200 ppm Pd(II) solution in a 50 mL conical tube. This adsorbent was promptly rinsed with deionized water and then resuspended in the eluent, which was a mixed solution of 0.01 M HCl and 0.01 M thiourea. A total of five repetitions were done for the adsorption and desorption cycles mentioned above. Following the proper dilution of the samples obtained from adsorption and desorption studies, the Pd(II) content of the samples was determined using an ICP-OES. The desorption efficiency was determined using the subsequent equation.

3. Results and Discussion

3.1. Characterization
3.1.1. TEM Image

To explore the shape and crystal structure of the CSH-based adsorbent, TEM examination of CSH and PEI-CSH was performed. CSH composites with a hierarchical structure can be obtained by hydrothermal reaction of the OS and fumed silica (Figure 1(a)). Moreover, a close-up image of the CSH lattice is presented in Figure 1(b), which exhibits a small grid shape, suggesting that the precursors are formed along calcium and oxygen sheets surrounded by tetrahedral silica chains. Moreover, CSH demonstrate that channels are arranged orderly and uniformly [34]. After crosslinking with PEI, the hierarchical structure disappeared as shown in Figure 1(c). In the magnified image (Figure 1(d).), the surface of PEI-CSH is covered with polymer, and only a partial lattice pattern is observed. It indicates that during the preparation process, the intrinsic properties of CSH were not destroyed, as well as the PEI functional ligands were successfully bound to the CSH surface.

3.1.2. XRD Analysis

In Figure 2, the entire XRD pattern peaks are strong, indicating that the substance is highly crystallized. The characteristic peaks of CSH occur at 20°–30° and 50.8° [35, 36]. The grafting of PEI to the CSH surface may be the cause of the observed drop in the main peak diffraction intensity for PEI-CSH. After adsorption process, one of the main peaks disappeared. The missing peak was located at 29.8°, which is considered to be the effect of Pd(II)-induced destructive interference [37].

3.1.3. FT-IR Analysis

The FT-IR is a crucial tool for analyzing changes in chemical bonds in materials as well as potential interactions between metal ions and the surface functional groups of adsorbents. The FT-IR spectra of CSH, PEI-CSH, and Pd-loaded PEI-CSH are presented in Figure 3. As shown in Figure 3(a), the peaks in the range of 1200–400 cm-1 represent the chemical bonds in the silica chains [38]. The peaks at 961, 641, and 443 cm-1 were assigned to Si-O (asymmetric stretching vibration), Si-O-Si (out-of-plane bending vibration), and O-Si-O (in-plane bending vibration), respectively [39]. After PEI coating, the peaks at 961, 643, and 443 cm-1 were shifted to 963, 643, and 451 cm-1, respectively (Figure 3(b)). There were four new peaks found at 1073, 902, 796, and 697 cm-1. The peak at 1073 cm-1 was assigned to the C-N stretching vibration of aliphatic amines [40]. The band associated with amines was seen in the 910-665 cm-1 range. Only primary and secondary amines were shown to have this robust, wide band, which was caused by N-H wagging [41]. Therefore, it can be explained that PEI was successfully crosslinked to the CSH surface. After the adsorption of Pd(II) (Figure 3(c)), the peaks at 1073, 902, 796, and 697 cm-1 shifted slightly, and the intensity also changed. This change can be considered a result of the involvement of the amine group in the adsorption process [42].

3.1.4. Zeta Potential

According to Figure 4, the zeta potential of CSH decreased from -5.32 to -26.70 mV, with the pH value increasing from 2 to 12. On the other hand, PEI-CSH showed a high positive charge of +32.77 mV at below pH 8 and negative charge at -1.40 mV at above pH 10. In addition, the isoelectric point (PI) of PEI-CSH was 9.85, which was present at a higher pH than that of CSH. Consequently, the surface of PEI-CSH is positively charged at a pH lower than PI, which can be considered due to the amine groups such as -NH+, -NH2+, and NH3+ in PEI coated on CSH.

3.2. Adsorption Mechanism

A large number of amine groups were produced on the surface of CSH as a result of PEI grafting onto CSH to generate PEI-CSH. The adsorption capacity of PEI-CSH for Pd(II) was significantly increased at pH 2 when amine groups were concentrated on the adsorbent surface (Figure 5(a)). The Pd(II) uptake of PEI-CSH was 99.54 mg/g, which is very high compared to that of OSP (6.97 mg/g) and CSH (4.38 mg/g). Interestingly, the difference in the amount of Pd(II) adsorption before and after the introduction of PEI into CSH is about 22.7-fold. As such, the presence/absence of PEI in the adsorbent largely affected the Pd(II) adsorption amount. To explain this result, it is necessary to check the form of Pd(II) at pH 2. As shown in Figure 5(b), Pd(II) exists as an anion in the form of PdCl42- in acidic conditions. Therefore, the anionic Pd(II) is likely to be bound with the positively charged amine groups in PEI-CSH through electrostatic attraction, which has been proved in our previous work [32].

3.3. Adsorption Isotherms and Modeling

To determine the maximal Pd adsorption capacity of PEI-CSH, isothermal adsorption studies were carried out at pH 2 (II). According to Figure 6, the PEI-Pd(II) CSH’s uptakes increased as Pd(II) concentrations rose before reaching their maximum adsorption capacity. Adsorption isotherm models can offer crucial details on the adsorption process, surface characteristics, and interactions between the adsorbent and adsorbate. The experimental data were described by Langmuir, Freundlich, Sips, Redlich-Peterson, and Temkin isotherm models (see Supporting Information (available here)), and the corresponding parameters are listed in Table 1.

The Langmuir and Sips models had greater coefficient of determination () values than the other models, indicating that they were more suited to explain the adsorption of PEI-CSH for Pd(II) [6]. According to the Langmuir model, PEI-CSH was adsorbed on Pd(II) in a monolayer [43]. The values fell between 0 and 1, indicating that PEI-CSH adsorption for Pd(II) was favorable [44]. According to the Sips model, the PEI-Pd(II) CSH’s adsorption process combines monolayer adsorption at high Pd(II) concentrations with diffusion at low Pd(II) concentrations [9]. Combining the Langmuir and Freundlich equations creates the Redlich-Peterson model. A value of 40.21 was determined for the Redlich-Peterson rate constant (). The result was close to 1, indicating that the Pd(II) isotherms are compatible with the Langmuir and Redlich-Peterson models and that they are near to the Langmuir form [45]. According to the Temkin model, all molecules in the layer will experience a linear drop in the heat of adsorption as the layer’s coverage increases due to the adsorbate-adsorbent interaction. As a result, the adsorption exhibits a consistent binding energy distribution up to a maximum level [46]. The exothermic nature of the adsorption process was suggested by the positive Temkin constant () value [9].

3.4. Adsorption Kinetics and Modeling

One of the key elements in determining the effectiveness of the overall adsorption process is adsorption kinetics, which also offers theoretical understanding of the reaction pathways and processes of adsorption [47]. To determine the time at which Pd(II) adsorption on PEI-CSH reaches equilibrium, the impact of contact time was assessed. The studies were conducted in an acidic environment () for 360 min at 25°C with an initial Pd(II) concentration of 200 mg/L. In the acidic setting, as shown in Figure 7, PEI-CSH adsorbed 95% of the Pd(II) during the first 120 min, reaching equilibrium at 180 min, demonstrating a very fast adsorption rate.

The pseudo-first-order (PFO), pseudo-second-order (PSO), Elovich, and intraparticle diffusion models (see Supporting Information) were used to explain kinetic data. Figure 7 and Table 2 show the fitting curves and accompanying parameters.

The parameters of kinetic models as well as values and are presented in Table 2. The experimental results confirmed that the PSO model, which had values near to unity, better suited the Pd(II) adsorption data when compared to the PFO and Elovich kinetic models. Additionally, the PSO model’s projected value for the Pd(II) uptake at equilibrium, , was quite similar to the experimental finding (99.67 mg/g). Since Pd(II) adsorption by PEI-CSH is a kinetic process, the PSO model proved effective in fitting the experimental data. It also suggests that chemisorption dominates physisorption during the adsorption process [48]. The chemisorption process is typically explained by the Elovich model [49]. The values of the Elovich model was 0.976, suggesting that chemisorption predominated in the adsorption process and that the model was acceptable for representing the kinetic adsorption process [49]. The three steps of the adsorption process are typically (1) film or external diffusion, (2) pore or intraparticle diffusion, and (3) adsorbate deposited on the adsorption site [50]. The rate-limiting phases of the adsorption process were identified using the intraparticle diffusion model. The results of vs. acquired from the Pd(II) adsorption experiment are displayed in Figure 7(b). Three separate stages were used to display the linear plot. Since the initial step did not go through the origin, it is likely that external diffusion and subsequently intraparticle diffusion were used preferentially to regulate the adsorption of Pd(II) on PEI-CSH until equilibrium was reached [51].

3.5. Reusability of PEI-CSH

For promising adsorbents, the capacity to be reused is a crucial characteristic. Adsorbent replacement cycles can be extended, and financial gain can be made if an exhausted adsorbent can be recycled. Each of the adsorption and desorption experiments was conducted up to five times. An acidified thiourea solution prepared by mixing 0.01 M HCl and 0.01 M thiourea was used as the eluent for desorbing Pd from the loaded adsorbent. The adsorption and desorption efficiencies were nearly constant at 100% across the five cycles, as illustrated in Figure 8. Desorption by thiourea is pH-dependent [52], and thiourea forms a coordination bond with metal ions at neutral pH but induces desorption by an anion-exchange mechanism with PdCl42- at acidic pH [32]. Since an acidified thiourea solution was used in this study, the desorption is considered to be due to anion exchange. It was also confirmed that the reusability of PEI-CSH was very excellent.

4. Conclusion

In summary, an oyster waste-based adsorbent, PEI-CSH, was developed, providing an alternative way for oyster shell waste recycling. According to the TEM image, the prepared CSH showed a hierarchical structure surface, and the PEI-CSH was covered with a polymer. As evidenced by XRD analysis, PEI-CSH was observed to have characteristic peaks of CSH, which was reduced in intensity by PEI. In addition, it was found through FT-IR analysis and one-point check adsorption experiments that the absorption performance of PEI-CSH was improved by amine groups. Modification of CSH with PEI also increased the point of zero charge to 9.85. These results revealed that the adsorbent was successfully prepared. The Langmuir model was more suitable for depicting adsorption of Pd(II) on PEI-CSH, and the maximum adsorption amount was 156.03 mg/g at pH 2. Kinetic experiment showed that the adsorption equilibrium for 200 mg/L of Pd(II) at pH 2 was reached within 180 min. According to the reusability research, PEI-CSH may be recycled at least five times without losing any of its adsorption capability. Overall, the PEI-CSH, fabricated from oyster shell waste, showed the possibility of eliminating anionic Pd(II) from a HCl solution.

Data Availability

The raw data used to support the findings of this study are available from the corresponding author upon request.

Conflicts of Interest

The authors declare that they have no conflicts of interest.

Acknowledgments

This research was supported by Basic Science Research Program through the National Research Foundation of Korea (NRF) funded by the Ministry of Education (NRF-2020R1A6A3A13068967 and NRF-2020R1F1A1065937).

Supplementary Materials

The following are the supplementary data to this article. (Supplementary Materials)