Microhardness Vickers of all textures before and after the hot stamping tests.
| Texture # | Position | Before hot stamping tests | After hot stamping tests | Mean HV | Standard deviation | Mean HV | Standard deviation |
| 1 | 1 | 565 | 20 | 538 | 25 | 2 | 565 | 32 | 573 | 19 | 3 | 597 | 19 | 592 | 30 | 4 | 574 | 23 | 534 | 32 |
| 2 | 1 | 486 | 40 | 590 | 32 | 2 | 597 | 18 | 572 | 16 | 3 | 534 | 35 | 576 | 4 | 4 | 525 | 23 | 568 | 23 |
| 3 | 1 | 571 | 33 | 501 | 30 | 2 | 587 | 38 | 603 | 29 | 3 | 581 | 17 | 581 | 19 | 4 | 580 | 29 | 616 | 21 |
| 4 | 1 | 607 | 19 | 563 | 12 | 2 | 591 | 22 | 563 | 9 | 3 | 584 | 51 | 565 | 29 | 4 | 530 | 20 | 569 | 32 |
| 5 | 1 | 514 | 13 | 568 | 35 | 2 | 571 | 17 | 595 | 28 | 3 | 564 | 34 | 568 | 19 | 4 | 583 | 32 | 585 | 18 |
|
As grinded | 1 | 548 | 26 | 592 | 28 | 2 | 570 | 40 | 595 | 28 | 3 | 564 | 25 | 568 | 19 | 4 | 568 | 27 | 585 | 35 |
|
|