Research Article
Inhibition Effect of Natural Pozzolan and Zinc Phosphate Baths on Reinforcing Steel Corrosion
Table 4
Water penetration depths, porosity, chloride penetrability, and pH of the investigated concrete.
| Curing time | Binder type | Water penetration depth (mm) | Porosity (%) | Chloride penetrability (Coulombs) | pH |
| 28 days | NP0 | 65 | 17.2 | 6278 | 12.65 | NP10 | 61 | 15.7 | 5891 | 12.34 | NP20 | 48 | 14.2 | 4367 | 12.08 | NP30 | 42 | 11.1 | 2915 | 12.01 |
| 90 days | NP0 | 53 | 14.4 | 3971 | 12.57 | NP10 | 43 | 12.2 | 3214 | 12.19 | NP20 | 29 | 9.7 | 1965 | 11.91 | NP30 | 22 | 6.8 | 1112 | 11.93 |
|
|