Research Article
[Retracted] Comparison of Microstructure and Mechanical Properties of A356/SiC Metal Matrix Composites Produced by Two Different Melting Routes
Table 10
Improved hardness of A356/SiC MMC by electromagnetic stir casting process.
|
A356/SiC MMC |
Sample number | Electromagnetic stir casting samples (ESCS) | Mechanical stir casting samples (MSCS) |
Improved hardness (BHN) | Hardness (BHN) | Variation (BHN) | Average Hardness (BHN) | Hardness (BHN) | Variation (BHN) | Average hardness (BHN) |
| 100% A356 + 0% SiC | 1 | 76 |
1 |
75.66 | 75 |
1 |
75.33 |
0.43% | 2 | 76 | 76 | 3 | 75 | 75 |
| 95% A356 + 5% SiC | 1 | 82 |
4.5 |
84.16 | 77.5 |
7.5 |
81.16 |
3.56% | 2 | 84 | 85 | 3 | 86.5 | 81 |
| 90% A356 + 10% SiC | 1 | 93 |
5.4 |
96.13 | 88 |
9 |
92.33 |
3.95% | 2 | 98.4 | 97 | 3 | 97 | 92 |
| 85% A356 + 15% SiC | 1 | 101 |
7 |
104.66 | 97 |
10 |
102 |
2.54% | 2 | 105 | 107 | 3 | 108 | 102 |
|
|