Performances of PSCs deposited under different temperatures: (a) 70°C, (b) 100°C, (c) 130°C, and (d) 160°C. The PEDOT:PSS films were deposited with IPA-diluted solution ((PEDOT:PSS) : IPA = 1 : 14) and 1% Zonyl FS-300 fluorosurfactant.

TEM (°C) (V) (mA/cm2)FF (%)η (%)

700.557.0539.41.57
1000.567.8047.02.01
1300.609.1749.12.55
1600.557.4534.71.40