Research Article
Synthesis and Characterization of Chemically Cross-Linked Acrylic Acid/Gelatin Hydrogels: Effect of pH and Composition on Swelling and Drug Release
Table 2
Equilibrium swelling ratio of AA/Gelatin hydrogels.
| Sample codes | Feed composition (AA/Gelatin) | Degree of cross-linking (EGDMA) % W/W | pH of the solution | 1.2 | 5.5 | 6.5 | 7.5 |
| U1 | 35.00/4.00 | 0.70 | 5.48 | 16.43 | 29.62 | 34.58 | U2 | 35.00/5.00 | 0.70 | 5.26 | 14.82 | 26.81 | 30.95 | U3 | 35.00/6.00 | 0.70 | 4.76 | 12.88 | 24.01 | 27.94 | U4 | 28.00/6.00 | 0.70 | 4.22 | 11.51 | 22.75 | 26.18 | U5 | 32.00/6.00 | 0.70 | 4.68 | 14.66 | 26.66 | 32.63 | U6 | 36.00/6.00 | 0.70 | 5.66 | 17.27 | 33.56 | 38.28 | U7 | 36.00/6.00 | 0.65 | 5.52 | 16.83 | 33.00 | 37.21 | U8 | 36.00/6.00 | 0.75 | 4.64 | 12.64 | 26.43 | 27.59 | U9 | 36.00/6.00 | 0.85 | 4.014 | 8.48 | 22.75 | 24.61 |
|
|