Research Article

Study of Na-Montmorillonite–Polyamide Fiber/Polypropylene Hybrid Composite Prepared by Reactive Melt Mixing

Table 3

Melting (), crystallization temperatures (), and enthalpies (, ) for different samples and crystallinity degree () obtained by DSC.

Sample (%)
(J/g)(°C)(J/g)(°C)

PP901619811642.4
PP/5 wt% t-PAfs7715989117.539
3 wt% Na-MMT87.9158.398.312043.6
5 wt% Na-MMT83.7158.598120.842.3
7 wt% Na-MMT81.716092.5119.542.1
3 wt% hyb87.7159.5102.312045.6
5 wt% hyb83.5159.3102.1120.344.7
7 wt% hyb83.1159.5100.1121.445.2