Research Article
Corrosion Study of Steel API 5A, 5L and AISI 1080, 1020 in Drill-Mud Environment of Iranian Hydrocarbon Fields
Table 4
Potentiodynamic results of tube casing (sample 2); path 1: anodic-cathodic, path2: reverse scan. Sample 2: Tube Casing.
| Media | V (path 1) | V (path 2) | mA/cm2 | Passivation |
| HCLβ0.1M |
β0.51
|
β0.53
| 2200 | β | HClβ1βM |
β0.5
|
β0.5
| 2200 | β | H2SO4β0.1βM |
β0.55
|
β0.5
| 2000 | After 1.5βV | H2SO4β1βM |
β0.47
|
β0.49
| 2300 | β | NaOHβ0.1βM |
β0.78
|
β0.31
| 4000 | β0.6 to 0.5βV | NaOHβ1βM |
β0.83
|
β0.33
| 900 | β0.7 to 0.9βV | Mud 1 |
β0.68
|
β0.6
| 600 | Narrow range | Mud 2 | β | β | β | β | Mud 3 |
β0.88
|
β0.64
| 600 | β | Mud 4 |
β0.7
|
β0.58
| 2000 | β | Mud 5 |
β0.74
|
β0.56
| 2000 | β |
|
|