Properties of High-Strength Flowable Mortar Reinforced with Palm Fibers
Table 4
Mechanical properties of mortar mixes.
| Index | Density | Compressive strength | Flexural strength | Density | Compressive strength | Flexural strength | Toughness Index I5 | Kg/m3 (7 days) | (MPa) (7 days) | (MPa) (7 days) | Kg/m3 (28 days) | (MPa) (28 days) | (MPa) (28 days) |
| M0 | 2300 | 42.1 | 6.52 | 2330 | 53.5 | 7.6 | 1.0 | M1 | 2260 | 46.3 | 6.88 | 2300 | 59.2 | 7.97 | 1.0 | M2 | 2250 | 47.1 | 7.11 | 2285 | 60.4 | 8.28 | 1.0 | M3 | 2240 | 47.9 | 7.54 | 2260 | 62.1 | 8.75 | 1.0 | M4 | 2240 | 44.3 | 6.88 | 2265 | 54.1 | 7.9 | 1.0 | M5 | 2235 | 42.3 | 5.94 | 2260 | 52.4 | 6.95 | 1.29 | M6 | 2210 | 41.4 | 5.33 | 2220 | 50.2 | 6.45 | 1.42 | M7 | 2180 | 33.7 | 5.35 | 2190 | 46.7 | 6.36 | 1.55 | M8 | 2175 | 29.1 | 4.88 | 2180 | 42.2 | 5.93 | 1.77 |
|
|