Research Article
Effect of Modifying Prosthetic Socket Base Materials by Adding Nanodiamonds
Table 1
Mechanical properties of the cured base material prepared with varying nanodiamond contents.
| Nanodiamond content (wt.%) | Compression strength | Tensile strength (MPa) | Elastic modulus (MPa) | Microhardness |
| 0.0 | 73.46 ± 1.56 | 39.23 ± 1.69 | 980.75 ± 78.38 | 9.17 | 0.2 | 74.20 ± 1.07 | 39.86 ± 1.35 | 1017.43 ± 52.12 | 10.53 | 0.5 | 77.55 ± 1.90 | 43.47 ± 1.21 | 1123.87 ± 28.71 | 13.15 | 1.0 | 79.32 ± 1.88 | 44.91 ± 1.39 | 1198.62 ± 48.40 | 13.29 |
|
|