Research Article
Comprehensive Evaluation of the Accelerated Aging Law of NEPE Propellants
Table 1
Gas release during accelerated aging of the NEPE propellant.
| 50°C | 60°C | 70°C | Time of storage (d) | Gas release | Time of storage (d) | Gas release | Time of storage (d) | Gas release | NOx (ppm) | CO2 (%) | NOx (ppm) | CO2 (%) | NOx (ppm) | CO2 (%) |
| 23 | 1.4 | 0.9 | 20 | 1.3 | 1.7 | 17 | 7.8 | 3.6 | 53 | 2.8 | 1.0 | 34 | 1.5 | 2.4 | 25 | 5.7 | 4.9 | 105 | 3.9 | 0.9 | 48 | 26 | 5.9 | 42 | 280 | 25.9 | 124 | 23 | 2.3 | 72 | 346 | 7.6 | 48 | 842 | 32 | 158 | 89 | 5.6 | 136 | 1508 | 15.7 | 52 | 1216 | 43 | 206 | 212 | 7.8 | 183 | 3860 | 23.7 | 62 | 5000 | 51 |
|
|