Order, amounts, weighing container, and formula weight of reagents for preparing 1000 mL of SBF.

OrderReagentAmountContainerFormula weight

1NaCl8.035 gWeighing paper58.4430
2NaHCO30.355 gWeighing paper84.0068
3KCl0.225 gWeighing bottle74.5515
4K2HPO4·3H2O0.231 gWeighing bottle228.2220
5MaCl2·6H2O0.311 gWeighing bottle203.3034
61.0M-HCl39 mLGraduated cylinder
7CaCl20.292 gWeighing bottle110.9848
8Na2SO40.072 gWeighing bottle142.0428
9Tris6.118 gWeighing paper121.1356
101.0M-HCl0~5 mLSyringe