Accelerated Weatherability of the Low-Density Polyethylene Nanocomposites with Silica, Clay, and Zinc Oxide

Table 4

Concentrated sunlight exposure (3 months outdoor exposure): average value (standard deviation).

SamplesMaximum load, NTensile strength, MPaMean extensibility (%)

LDPE control363.23 (1.84)9.46 (0.10)160.75 (3.89)
LDPE 5 wt% ZnO374.16 (2.35)9.72 (0.07)147.98 (2.99)
LDPE 5 wt% silica387.49 (2.91)10.09 (0.09)140.63 (3.90)
LDPE 5 wt% clay368.64 (1.41)9.61 (0.07)150.44 (3.33)