XRD results and TEM grain size for the 0.5 Er annealed powders.

Powder sampleLattice parameter (Å)Mg in matrix (at.%)Grain size, XRD (nm)Microstrain (%)Correlation coefficient, Grain size, TEM (nm)Number of grains,

Milled4.0647 ± 0.00044.87190.1060.9317 ± 0657
150°C4.0562 ± 0.00252.72210.0660.8922 ± 1468
250°C4.0519 ± 0.00041.6223 0.0540.9418 ± 1372
400°C4.0530 ± 0.00061.9027 0.060.9718 ± 1328
450°C4.0544 ± 0.00062.26350.0890.9332 ± 2301
500°C4.0537 ± 0.00052.08410.0780.8554 ± 4300