An Effective Method for Hybrid CNT/GNP Dispersion and Its Effects on the Mechanical, Microstructural, Thermal, and Electrical Properties of Multifunctional Cementitious Composites
Table 7
Test results of the cementitious composites according to the standard procedures.
Name of sample
Flow values1 (mm)
Flexural strength2 (N/mm2)
Compressive strength2 (N/mm2)
Apparent porosity3 (%)
Ultrasonic wave time passing4 (μs) for 150 kHz
Dry bulk density5 (kg/m3)
Longitudinal
Transverse
Plain mortar
183.2
6.9
43.9
19
36.40
9.70
2125
Plain mortar+5%S+TBP
191.7
7.1
44.9
15.9
36.21
9.51
2130
1%CG+5%S+3H+TBP+40°C
118.4
7.8
47.8
13.6
34.10
9.34
2135
Plain mortar+10%P+TBP
198.2
7.2
44.2
13.9
35.88
9.38
2130
1%CG+10%P+3H+TBP+40°C
131.5
8.3
51.1
11.4
32.97
8.93
2140
1BS EN 1015-3; 2BS EN 196-1:1995; 3ASTM C20; 4BS EN 12504-4; 5BS EN 1015-10:1999.