AA4015+TiC+B4C processed composite hardness and S/N ratio value.

Exp no.12345678

Sintering time (hr)1.751.751.752222.252.25
Sintering temperature (°C)610620635610620635610620
Compaction pressure (MPa)250300350300350250350250
Hardness (Hv)2628.8229.6228.7929.1825.8230.2227.64