Research Article
Preparation and Characterization of Talc Filled Thermoplastic Polyurethane/Polypropylene Blends
Table 1
DMA results of the neat TPU, PP, TPU/T and PP/T composites, and unfilled and talc filled TPU/PP blends.
| Sample | (°C, ) | (°C, ) | (GPa) at 25°C | (°C) |
| TPU 100/0 | −27.3 | — | 0.1 | — | TPU/T 100/5 | −21.7 | — | 0.2 | — | PP 100/0 | — | 24.3 | 2.3 | 57.2 | PP/T 100/5 | — | 26.4 | 2.8 | 69.4 | TPU/PP 80/20 | −22.2 | — | 0.2 | — | TPU/T/PP 80/5/20 | −21.1 | — | 0.5 | — | TPU/PP 50/50 | −21.2 | 16.6 | 1.0 | 72.3 | TPU/T/PP 50/5/50 | −18.0 | 18.2 | 1.2 | 77.0 | TPU/PP 20/80 | −26.7 | 20.7 | 1.9 | 75.3 | TPU/T/PP 20/5/80 | −20.3 | 22.5 | 2.0 | 76.7 |
|
|