Research Article

Dynamic Compressive and Tensile Characteristics of a New Type of Ultra-High-Molecular Weight Polyethylene (UHMWPE) and Polyvinyl Alcohol (PVA) Fibers Reinforced Concrete

Table 6

Static tensile properties of fiber concrete of each group.

Group numberPeak load (KN)Average peak load (KN)Tensile strength (MPa)Elastic modulus (GPa)
123

016.5316.6116.4216.523.8428.6
P-0.617.1517.4317.0917.224.0127.5
U-0.617.3817.5417.4317.454.0627.1
P-1.217.5217.6717.5817.594.0926.4
U-1.217.7317.8517.7617.784.1425.8
P-1.817.8617.8317.8717.894.1625.2
U-1.818.0518.0718.1018.074.2024.7
P-2.418.0218.1618.0818.094.2123.9
U-2.418.2218.3618.3118.304.2623.4