Chemical composition and mechanical properties of AFNOR 15CDV6 steel [2].
(a) Composition (wt%).

CSi (max)MnP (max)S (max)CrMoV

0.150.170.900.0300.0131.500.900.32

(b) Mechanical properties in the hardened and tempered condition*

UTS (MPa)0.2% PS (MPa)% ElongationCharpy U-notch impact energy (kJ/m2)Hardness BHN

980–1175830–9808–12650–700360

*Austenitized at 980°C, quenched in oil, tempered at 650°C, quenched in oil.