Ultrasonic, absorption, and voids for HSFM.

Mix typeSF (%)PF (%)BF (%)Ultrasonic (m/s) 90 daysAbsorption (%) 90 daysVoids (%) 90 days

M0377010.6220.3
M10.25386010.5419.86
M20.50392010.1419.56
M30.7540309.9319.17
M41.040709.8119.10
M51.2542809.5618.98
M61.5041909.3218.53
M71.7541309.2118.38
M82.041109.116.78
M91.750.2541409.1817.73
M101.500.5041009.2218.14
M111.250.7540809.4518.74
M121.01.040609.618.92
M131.00.500.5040209.5418.81
M141.250.500.2540809.3618.37
M151.250.250.5041009.2818.22
M161.500.250.2541609.1417.32